Q/BQB 440-2023_English: PDF (Q/BQB440-2023)
Standard ID | Contents [version] | USD | STEP2 | [PDF] delivered in | Standard Title (Description) | Status | PDF |
Q/BQB 440-2023 | English | 879 |
Add to Cart
|
5 days [Need to translate]
|
Prepainted steel sheet and strip
| |
Q/BQB 440-2023
|
Q/BQB 440-2018 | English | 100 |
Add to Cart
|
0--9 seconds. Auto-delivery
|
Prepainted steel sheets and strips
| |
Q/BQB 440-2018
|
Q/BQB 440-2014 | English | 215 |
Add to Cart
|
0--9 seconds. Auto-delivery
|
Prepainted steel sheets and strips
| Obsolete |
Q/BQB 440-2014
|
Q/BQB 440-2009 | English | 749 |
Add to Cart
|
3 days [Need to translate]
|
Color coated steel sheet and strip
| Obsolete |
Q/BQB 440-2009
|
Standard ID | Q/BQB 440-2023 (Q/BQB440-2023) | Description (Translated English) | Prepainted steel sheet and strip | Sector / Industry | Chinese Industry Standard | Classification of Chinese Standard | QBQ | Word Count Estimation | 25,239 | Date of Issue | 2023-04-09 | Date of Implementation | 2023-07-01 | Standard ID | Q/BQB 440-2018 (Q/BQB440-2018) | Description (Translated English) | Prepainted steel sheets and strips | Sector / Industry | Chinese Industry Standard | Classification of Chinese Standard | QBQ | Word Count Estimation | 5,520 | Administrative Organization | Baoshan Iron and Steel Co., Ltd. | Standard ID | Q/BQB 440-2014 (Q/BQB440-2014) | Description (Translated English) | Prepainted steel sheets and strips | Sector / Industry | Chinese Industry Standard | Classification of Chinese Standard | QBQ | Word Count Estimation | 15,152 | Drafting Organization | BaoSteel Group | Administrative Organization | BaoSteel Group |
Q/BQB 440-2018
BQB
ENTERPRISE STANDARD OF
BAOSHAN IRON AND STEEL CO., LTD
Steel sheet and steel strip with colored coating
Issued on. February 02, 2018
Issued by. Baoshan Iron and Steel Co., Ltd.
Table of Contents
Self-commitment ... 3
Technical indicator 1 ... 4
1 Chemical composition ... 5
2 Coating performance ... 5
3 Inspection and testing ... 7
Self-commitment
The contents of the Q/BQB 440-2018 “Steel sheet and steel strip with colored
coating” which are prepared and published by our company are in compliance
with the requirements of relevant national laws and regulations, mandatory
standards and relevant industrial policies, meanwhile it is approved by the
corporate’s legal representative in accordance with the prescribed procedures.
The products which are produced by our company meet the technical
requirements as specified in this standard, the standard number is clearly
indicated on the corresponding product packaging. Our company is responsible
for the truthfulness, accuracy and legality of the public information, assumes full
legal responsibility for the consequences of the implementation of this standard.
Baoshan Iron and Steel Co., Ltd.
2018-02-02
......
Q/BQB 440-2014
Q/BQB
SUPPLY TECHNICAL CONDITIONS
OF BAOSHAN IRON & STEEL CO., LTD.
Replacing Q/BQB 404-2009
Prepainted steel sheets and strips
Issued on. October 18, 2014 Implemented before. March 31, 2015
Issued by. Baoshan Iron & Steel Co., Ltd.
Table of Contents
1 Scope ... 4
2 Normative references ... 4
3 Terms and definitions ... 5
4 Classifications and codes ... 6
5 Order required information ... 7
6 Size, appearance, weight and tolerance ... 8
7 Technical requirements ... 8
8 Inspection and test ... 13
9 Packaging, marks and inspection documents ... 15
10 Transport, storage, processing ... 15
11 Numerical correction rule ... 15
12 Description of the corrosion of the environment of use ... 16
13 Selections of prepainted steel sheet ... 16
14 Prepainted steel sheet’s storage, transport and loading-unloading ... 16
15 Prepainted steel sheet’s processing ... 16
16 Life to the first major maintenance and durability of prepainted steel
sheet ... 16
17 Air exposure test field of prepainted steel sheet ... 16
Annex A (Informative) Description of the corrosion of the environmental of use
... 17
Annex B (Informative) Selection of prepainted steel sheet ... 21
Annex C (Informative) Storage, transport and loading-unloading of prepainted
steel sheet ... 25
Annex D (Informative) Processing of prepainted steel sheet ... 27
Annex E (Informative) Life to the first major maintenance and durability of
prepainted steel sheet ... 29
Annex F (Informative) Air exposure test field of prepainted steel sheet ... 30
Prepainted steel sheets and strips
1 Scope
This Technical Conditions specifies the terms and definitions, classifications
and codes, size, appearance, weight, technical requirements, inspection and
testing, packaging, marking and inspection documents of prepainted steel
sheet and strips (hereinafter referred to as prepainted steel sheet).
This Technical Conditions is applicable to the building prepainted steel sheets
that are manufactured by Baoshan Iron & Steel Co., Ltd., of thickness of 0.22
mm ~ 2.0 mm. The industries of home appliance, furniture, steel window can
refer to use.
2 Normative references
The following referenced documents are indispensable for the application of
this document. For dated references, only the edition cited applies. For
undated references, the latest edition of the referenced document (including
any amendments) applies.
GB/T 1766-2008, Paints and Varnishes-Rating Schemes of Degradation of
Coats
GB/T 8170-2008, Rules of rounding off for numerical values & expression
and judgement of limiting values
GB/T 13448-2006, Test methods for prepainted steel sheet
GB/T 15957-1995, Corrosivity classification of atmospheric environment
GB/T 19292.1-2003, Corrosion of metals and alloys - Corrosivity of
atmospheres - Classification
Q/BQB 400, Packaging, marks and inspection documents of cold-rolled
products
Q/BQB 420, Hot-dip galvanized / zinc-iron alloy coated steel sheet and
strip
Q/BQB 425, Hot-dip galvanized alloy steel sheet and strip
Q/BQB 430, Galvanized steel sheet and strip
3 Terms and definitions
3.1 prepainted steel sheet
the product of which the organic coating (the top side is at least two layers) is
continuously coated on the surface-pretreated substrate and then is baked
and cured
3.2 steel substrate
the steel strip used for coating painting
3.3 top side
usually referring to the higher demanding side on color, coating performance,
surface quality in the two sides of prepainted steel sheet; when delivered in
roll, it usually refers to the outside of the prepainted steel coil
3.4 bottom side
the opposite side to the top side of prepainted steel sheet
3.5 building exterior applications
the applications mainly affected by building external atmosphere
3.6 building interior applications
the applications mainly affected by building internal atmosphere
3.7 hardness
the ability of coating to resist to scratch, friction, collision, press and other
mechanical effects
3.8 flexibility
the ability of the coating to co-deform with the substrate without damage
3.9 adhesion
the firmness between coatings or between coating and substrate
3.10 life to the first major maintenance
the interval FROM the end of production TO the time when the performance
of original coating degrades then major maintenance must be carried out so
as to continue protecting the substrate
comply with the provisions of Table 4. Special requirements for pencil
hardness shall be negotiated at the time of order.
7.2.3 Coating gloss
7.2.3.1 The coating gloss is represented by 60° mirror gloss. The gloss is
divided into low, medium and high grades. The nominal value of gloss at all
grades shall be in accordance with the provisions of Table 4.
7.2.3.2 The gloss of three samples shall comply with corresponding
provisions of Table 4. For low gloss coating, the gloss tolerance is ± 3 gloss
units. For medium gloss coating, the gloss tolerance is ± 10 gloss units. For
high gloss coating, the gloss tolerance is 0 ~ -10 gloss units.
7.2.3.3 The difference in gloss per batch of product shall not exceed 10
gloss units.
7.2.4 Coating flexibility / adhesion
7.2.4.1 The coating flexibility / adhesion is usually evaluated by bending test
and reverse impact test. If the cross-grid test, cup sudden test, etc. are
required for further evaluation, it shall be negotiated at the time of order.
7.2.4.2 Bending test
7.2.4.2.1 Three sample values of bending test shall comply with the
corresponding provisions of Table 4. Special requirements for bending test
shall be negotiated at the time of order.
7.2.4.2.2 After the bending sample is stripped off by tape, there shall be no
coating peeling off at the bend, excluding the coating falling off within 10 mm
from the sample edges. If non-visible cracks are required at the bend, it shall
be negotiated at the time of order.
7.2.4.2.3 The prepainted steel sheets are usually supplied in A-level T-bend.
B-level T-bend performance shall be negotiated at the time of order. Steel
windows are usually supplied in accordance with the B-level T-bend. For
prepainted steel sheets of which the designations are TS550GD+Z and
TS550GD+AZ, T-bend performance is not required. If there are special
requirements for T-bend performance, it shall be negotiated at the time of
order.
7.2.4.3 Reverse impact test
7.2.4.3.1 The minimum value of reverse impact test’s three samples shall
comply with the provisions of Table 4. Special requirements for impact energy
shall be negotiated at the time of order.
7.2.4.3.2 After the reverse impact test sample is peeled off by tape, there
shall be no coating peeling off in the deformation area. If non-visible cracks
are required at the deformation area, it shall be negotiated at the time of
order.
7.2.4.3.3 For prepainted steel sheets of which the thickness is less than
0.40 mm and designations are TS550GD+Z, TS550GD+AZ, the reverse
impact test is not required.
7.2.5 Coating durability
7.2.5.1 The coating durability is usually evaluated by the resistance to
neutral salt spray test or the ultraviolet lamp accelerated weathering test. If
the xenon lamp accelerated weathering test, heat resistance and resistance
to sulfur dioxide hot and humid test are required for further evaluation, it shall
be negotiated at the time of order.
7.2.5.2 Resistance to neutral salt spray test
7.2.5.2.1 The time of the resistance to neutral salt spray test of coating shall
comply with the provisions of Table 4. Special requirements for test time shall
be negotiated at the time of order.
7.2.5.2.2 Within the specified time of neutral salt spray test, the bubble
density level and bubble size rating of unmarked sample shall not exceed
grade 3 specified in Table 21 of GB/T 1766.
7.2.5.3 Ultraviolet lamp accelerated weathering test
7.2.5.3.1 The time of ultraviolet lamp accelerated weathering test of coating
shall comply with the provisions of Table 4. Special requirements for test time
shall be negotiated at the time of order.
7.2.5.3.2 Within the test time specified in Table 4, the sample should be free
of foam, cracks. Powdery shall not exceed grade 1 specified in GB/T 1766.
7.2.5.3.3 When the coating is polyester and silicon-modified polyester, it is
usually evaluated with UVA-340. If UVB-313 is used for evaluation, it shall be
indicated at t...
......
|